Abstract
Photocatalysis is an area of immense research for finding suitable benign photocatalyst for fast
and complete mineralization of environmental pollutants such as pesticides and polycyclic
aromatic hydrocarbons. Undeniably, TiO2 specifically P25-TiO2 which is commercially available
TiO2 have been widely studied for the same, however suffers from some disadvantages such as
crystal phase transformation at high temperature, UV-light sensitivity and low percentage of
mineralization of above mentioned molecules, limiting its utilization. This creates a scope to
modify TiO2 and/or to find other Ti-O based materials possessing similar physicochemical
properties but with improved photocatalytic activity for decomposition of aforementioned
molecules. In this context, present work considers the synthesis of titania/titanate nanostructures
in different sizes, shapes, crystal structures which were loaded by metals/coated by SiO2 of
different shell thickness and studied for the decomposition of some pesticides and polycyclic
aromatic hydrocarbons to CO2 in comparison to P25-TiO2.
Titania based nanocatalysts such as sodium titanates of different morphology having
superior surface properties are getting wide importance in photocatalytic research. Despite
having sodium (Na) content and its high temperature synthesis (that generally deteriorate the
photoactvity), these Na-titanates often exhibit better photoactivity than P25-TiO2 catalyst.
Hence, chapter-3 demonstrated the influence of crystal structure, BET surface area, surface
charge, zeta potential and metal loading on the photocatalytic activity of as-prepared sodium
titanate nanotubes and titania nanorods. Straw like hollow orthorhombic nanotube
(Na2Ti2O5·H2O) particles (diameter = 9-12 nm and length = 82-115 nm) and rice like anatase
nanorod particles (diameter = 8–13 nm and length = 81-134 nm) were obtained by the
hydrothermal treatment of P25-TiO2 with NaOH, which in fact, altered the net surface charge of
these as-prepared nanoparticles. The observed zeta potential = -2.82 (P25-TiO2), -13.5
(nanotubes) and -22.5 mV (nanorods) are significantly altered by the Ag and Cu deposition. It
has been found here that nanotube particles displayed best photocatalytic activity for
imidacloprid insecticide degradation to CO2 formation under UV irradiation because of its
largest surface area 176 m2g-1 among the studied catalysts.
Sodium titanate nanotubes having higher photocatalytic activity than P25-TiO2 was
photodeposited by Ag-nanoparticles (0.2-1.0 wt%, 3-5 nm) and studied for decomposition of
imidacloprid in chapter-4. The enhanced pseudo-first order rate constants for photooxidation of
v
imidacloprid to CO2 were found to increase with increase in Ag-photodeposition onto nanotubes
upto 0.5 wt%. The investigation for the fate of heteroatoms (N, O and Cl) present in imidacloprid
showed increase in formation of inorganic ions (nitrate, nitrite and chloride) with time of
photooxidation as confirmed by Ion chromatograph. Despite complete degradation of
imidacloprid in 180 min, its mineralization to CO2 was 70% due to formation of some persistent
heteroatom containing intermediates as revealed by time dependant GC-MS study. Based upon
these results, a probable pathway for mineralization of imidacloprid and a chemical mass
balanced equation in relation to theoretically expected equation after its complete mineralization
is proposed and described.
Preparation of crystalline monoclinic stick like sodium titanate nanorods by calciantion
(at 800 oC) of sodium titanate nanotubes, having much less surface area (21 m2g-1) but higher
average relaxation time of excited charge carriers to that of nanotubes and P25-TiO2, as
confirmed by XRD, TEM and time resolved photoluminescence decay studies is presented in
chapter-5. These nanostructures were modified by Au-photodeposition (0.5 and 2.0 wt%) and
studied for photoreduction of m-dinitrobenzene and photooxidation of sulfosulfuron. The
selective formation of m-diaminobenzene by photoreduction of m-dinitrobenzene was
comparable to sodium titanate nanorods (89.5 ± 0.5%) and P25-TiO2 (98.2±0.8%), whereas Audeposition
(0.5 and 2 wt%) notably altered the products (m-nitroaniline and m-diaminobenzene)
distribution after 8 h of UV-light irradiation, confirmed by GC-MS analysis. This high
photoactivity of as-prepared nanorods could be credited to better delocalization and longer
relaxation lifetime (68 ìs) of photoexcited e-/h+ pairs along the length of crystalline sodium
titanate nanorods than P25-TiO2 (45 ìs). The photooxidation of sulfosulfuron herbicide
(1000 ppm) and corresponding CO2 formation was found to be highest with sodium titanate
nanotubes due to the presence of more hydroxyl groups over the largest surface area which was
found to dominates over its least relaxation lifetime (41 ìs).
An understanding of the collective influence of Au-loading and calcination for the change
in crystal-structure, morphology, phase composition and their photocatalytic-activity of titanatenanostructures
is investigated in chapter-6. Bare and Au-loaded (Au+3, Auo and Aunanoparticles)
sodium-titanate-nanotubes were calcined in air at 800 oC, where TNT having
BET-surface-area 176 m2g-1 transformed into sodium-titanate-nanorods of surface-area of 21
m2g-1 while Au-loaded nanotubes led to a variety of fragmented-particles having different
vi
crystal-structures, surface-area (21-39 m2g-1) and sizes (50-75 nm), attributed to the strain
induced thermal-decomposition of nanotubes after Au-loading. Their comparative
photocatalytic- activities were evaluated by the photooxidation of insecticide imidacloprid with
identification of intermediates formed during its mineralization to CO2 under UV-light
irradiation, where 0.5 wt% Auo-deposited-nanotubes followed by calcination showed highest
photocatalytic-activity in-contrast to other catalysts. These results are well explained in
correlation with their crystal phase, surface-area, size, shape, and relaxation time of photoexcited
electron-hole pairs.
An important finding of the present work is delivered by chapter-7, showing complete
retention (> 98%) of anatase TiO2 crystalline phase after high temperature (800 oC) treatment of
rice-like TiO2 nanorods relative to 100% conversion of the rutile phase after calcination of P25-
TiO2 under similar conditions. In addition to XRD, the existence of anatase phase at > 800 oC
was confirmed by the presence of its characteristic vibrational bands (144, 395, 513 and 639
cm-1) in the Raman spectra. It was found that TiO2 nanorods undergo fragmentation to a highly
crystalline irregular morphology (60-70 nm), nanopolygons (91-110 nm) and smaller rod-shaped
particles (length = 60-110 nm and diameter = 7-12 nm), accompanied by a gradual increase in
their crystallite size (from 16 to 40 nm) and decrease in surface area (from 79 to 31 m2 g-1) with
increased calcination temperatures from 200 to 900 oC. This TiO2 anatase phase displayed
enhanced photocatalytic oxidation rate (~2–11 times higher than rutile TiO2) for methyl
parathion (a neurotoxic pesticide) degradation to various intermediate products and ultimately to
CO2, whereas 1.0 wt% Au–TiO2 significantly improved the photoactivity.
Preparation of SiO2 coated TiO2 particles having different thickness of silica shell and
their comparative photocatalytic activity, for the photooxidation of naphthalene (20 ppm) and
anthracene (20 ppm) is shown in chapter-8. The presence of SiO2 over TiO2 was demonstrated
by FT-IR analysis, showing peaks corresponding to Si-O-Si (1081 cm-1) and Si-O-Ti (950 cm-1)
bonds. HR-TEM analysis confirmed the presence of SiO2 in as-prepared samples of shell
thickness 12-15 nm and > 50 nm, with Si amount (0.8-4.2 at.%) determined by EDS analysis.
Increase in thickness of SiO2 increases the surface area of TiO2 (69-235 m2g-1) which in turn
improves the adsorption of naphthalene/anthracene. However, the observed trend for the
photocatalytic activity is in contrast to the trend of adsorption studies, where, as-prepared
samples with highest surface area exhibited the least photocatalytic activity, while catalyst of
vii
least surface area (among silica coated samples) showed highest activity for degradation of
naphthalene and anthracene to CO2. Despite complete degradation of naphthalene and
anthracene, an incomplete mineralization occurred, ascribed to the existence of various
intermediates identified by GC-MS analysis.
Influence of TiO2 morphology and Au-loading (1.0 wt%) for photocatalytic activity
under UV- and Sun-light is delivered in chapter-9. The phase composition obtained by XRD
study of as-prepared TiO2 nanowires (anatase = 72%, rutile = 28%) was found to be almost
similar to commercially available P25-TiO2 (anatase = 70%, rutile = 30%). SEM analysis
revealed the presence of elongated nanostructures corresponding to length = 1.9-8.0 ìm and
diameter = 80-270 nm for bare sample. The TEM analysis for Au-loaded TNW showed uniform
dispersion of Au nanoparticles (3-6 nm) over elongated nanostructures having dimension in
agreement with the SEM analysis. Time resolved analysis revealed that by changing the shape
from nearly spherical (P25-TiO2) to lengthy nanostructures, the recombination time of e-/h+ pair
increases from 45 to 64 ìs and was 79 ìs after Au-loading on the later. The photocatalytic
activity of bare and Au-loaded TiO2 nanowires under UV- and Sun-light was assessed by
decomposition of propiconazole to CO2, where Au-loaded TNW always exhibited higher activity
than P25-TiO2, and various intermediates after its complete degradation were identified by GCMS
analysis.
Description
Ph.D, SCBC, Thesis